Nitronic® 60

Nitronic® 60

Nitronic® 60 is known for its excellent galling resistance, even at elevated temperatures. The additions of 4% silicon and 8% manganese inhibit wear, galling, and fretting. It is commonly used for various fasteners and pins that require strength and resistance to galling. It maintains decent strength up to temperatures of 1800°F and has oxidation resistance similar to that of 309 stainless steel. The general corrosion resistance is between that of 304 and 316 stainless steel.

Chemistry

 NiCrMnSiCNSPFe
MIN 8.0 16.0 7.0 3.5 - 0.08 - - -
MAX 9.0 18.0 9.0 4.5 0.10 0.18 0.03 0.06 Balance

Specifications

ASME SA 193, ASME SA 479
ASTM A 193, ASTM A 193 Class 1C, ASTM A 276, ASTM A 479
UNS S21800

Inventory

Nitronic® 60 Round Bar

Common Trade Names

N60 Stainless

Features

  • Wear and galling resistant alloy

Applications

  • Fasteners
  • Pins and bushings
  • Wear rails
  • Roller bearings
  • Pump components

Physical Properties

Density: 0.275 lb/inch3
Electrical Resistivity: 589 ohm circ-mil/ft

Temperature, °F 70 200 400 600 800 1000 1200 1400 1600 1800
Coefficient of Thermal Expansion, in/in°F x 10-6 - 8.8 9.2 9.6 9.8 10.0 10.3 10.5 10.7 11.0
Modulus of Elasticity,
psi X 106 STA
- 26.2 - - - - - - - -

* 70°F to indicated temperature.

Mechanical Properties

Minimum Specified Properties, ASTM A 276 Bar

Ultimate Tensile Strength, ksi 95
0.2% Yield Strength, ksi 50
Elongation, % 35
Reduction of Area, % 55
Hardness MAX, Brinell 241

Typical Tensile Properties Annealed Bar ¾ - 1"

Temperature, °F 68 200 400 600 800 1000 1200 1400 1600
Ultimate Tensile Strength, ksi 106.5 98.2 84.4 80.5 78.3 75.4 66.6 49.8 30.2
0.2% Yield Strength, ksi 56.5 44.4 32.8 29.7 29.0 28.0 28.1 25.3 16.4
Elongation, 2% 61.7 63.3 64.0 59.6 65.5 52.2 48.2 47.1 72.8

Nitronic® is a registered trademark of AK Steel.