Excellent resistance to oxidation under mildly cyclic conditions through 2000°F characterizes 310. Because of its high chromium and medium nickel contents, 310 has good resistance to sulfidation and other forms of hot corrosion. 310 is widely used in moderately carburizing atmospheres such as encountered in petrochemical environments. The more severely carburizing atmospheres of industrial heat treating furnaces require RA330® or RA333®. 310 is not suggested for the severe thermal shock of repeated liquid quenching.
Often in many product forms, the grain size and carbon content can meet both the 310S and 310H requirements. 310 is often used at cryogenic temperatures, with excellent toughness to -450°F, and low magnetic permeability. 310 has a machinability rating of 42% relative to AISI B1112 steel. When using high speed steel tooling, this equates to about 70 surface feet per minute. Forming operations should be performed at room temperature whenever possible. Welding with AWS E310-15 electrodes or ER310 bare wire is suggested.
310 Stainless
310 Plate, 310 Sheet, 310 Coil, 310 Bar, 310 Pipe, 310 Welding Products, 310 Tubing, 310 Rod Coil
UNS S31008, UNS S31009, Werkstoff 1.4845, EN 10095
ASTM: A 240, A 276, A 312, A 479
ASME:SA-240, SA-479, SA-312
AMS:5521, 5651
| Cr | Ni | C | Si | Mn | P | S | Mo | Cu | Fe | |
|---|---|---|---|---|---|---|---|---|---|---|
| MIN | 24.0 | 19.0 | - | - | - | - | - | - | - | - |
| MAX | 26.0 | 22.0 | 0.08 | 0.75* | 2.0 | 0.045 | 0.03 | 0.75 | 0.5 | Balance |
* ASTM specification 1.50 max Si.
Density: 0.284 lb/inch3
Melting Point: 2470 - 2555°F
| Temperature, °F | 70 | 1000 | 1200 | 1400 | 1600 | 1800 | 2000 |
| Coefficient* of Thermal Expansion, in/in°F x 10-6 | - | 9.5 | 9.8 | 10.05 | 10.15 | 10.3 | 10.6 |
| Thermal Conductivity Btu • ft/ft2 • hr • °F |
7.6 | 13.6 | 15.2 | 16.8 | 18.4 | 20.0 | - |
| Modulus of Elasticity, Dynamic psi x 106 | 29.0 | 23.0 | 21.8 | 20.5 | 19.2 | - | - |
* 70°F to indicated temperature.
Representative Tensile Properties
| Temperature, °F | 10 | 1000 | 1200 | 1400 | 1600 |
| Ultimate Tensile Strength, ksi | 80.0 | 67.8 | 54.1 | 35.1 | 19.1 |
| 0.2% Yield Strength, ksi | 35.0 | 20.8 | 20.7 | 19.3 | 12.2 |
| Elongation, % | 52 | 47 | 43 | 46 | 48 |
Typical Creep- Rupture Properties
| Temperature, °F | 1200 | 1400 | 1600 | 1800 |
| Minimum Creep 0.0001%/Hr, ksi | 14.9 | 3.3 | 1.1 | 0.28 |
| 10,000 Hour Rupture Strength, ksi | 14.4 | 4.5 | 1.5 | 0.66 |