Nitronic 50 (XM-19)

Nitronic® 50 is a high strength and good corrosion resistant austenitic stainless steel. It has nearly double the yield strength of 304 and 316 stainless steel and has better corrosion resistance than 317L stainless steel. N50 Stainless remains non-magnetic even after being severely cold worked. It maintains strength at high temperatures as well as sub-zero temperatures.

Common Trade Names

N50 Stainless

Inventory

N50 Round Bar

Specifications

UNS S20910, Werkstoff 1.3964, EN 1.3964, ASTM A 276, NACE MR0175, ISO 15156-3

Chemical Composition, %

 NiCrMoMnSiCNSPCbVFe
MIN 11.5 20.5 1.5 4.0 - - 0.2 - - 0.1 0.1 -
MAX 13.5 23.5 3.0 6.0 1.0 0.06 0.4 0.03 0.045 0.3 0.3 Balance

Features

  • High strength austenitic alloy
  • Good corrosion resistance

Applications

  • Seawater pump shafts
  • Heat exchangers
  • Pressure vessels
  • Marine hardware

Physical Properties

Density: 0.285 lb/inch3
Melting Range: 2579-2642°F
Electrical Resistivity: 492 ohm circ-mil/ft

Temperature, °F 70 200 300 400 600 800 900 1000 1200 1400
Coefficient of Thermal Expansion, in/in°F x 10-6 - 9.0 - 9.2 9.6 9.9 - 10.2 10.5 10.8
Thermal Conductivity
Btu • ft/ft2 • hr • °F
108 - 108 - 124 - 141 - 160 -
Modulus of Elasticity,
psi X 106 STA
- 26.2 - - - - - - - -

* 70°F to indicated temperature.

Mechanical Properties

Minimum Specified Properties, ASTM A 276 Bar

Ultimate Tensile Strength, ksi 100
0.2% Yield Strength, ksi 55
Elongation, % 35
Reduction of Area, % 55

Typical Tensile Properties

Temperature, °F -320 -100 75 200 400 600 800 1000 1200 1350 1500
Ultimate Tensile Strength, ksi - - 117 107 96 92 89 84 74 66 52
0.2% Yield Strength, ksi - - 60 50 38 35 34 32 31 31 30
Elongation, 2% - - 45 43.5 43.5 42.5 43.5 41 38 37 41
Impact Strength, ft-lbs 50 115 170 - - - - - - - -

Nitronic® is a registered trademark of AK Steel.


Back to Top
Page Description: Rolled Alloys stocks N50 Round Bar
Keywords: N50,n-50,nitronic 50,N50 bar,n-50 bar,nitronic 50 bar,N50 round bar,n-50 round bar,nitronic 50 round bar, UNS S20910, AMS 5764, XM-19, Werkstoff 1.3964