Nitronic® 60 is known for its excellent galling resistance, even at elevated temperatures. The additions of 4% silicon and 8% manganese inhibit wear, galling, and fretting. It is commonly used for various fasteners and pins that require strength and resistance to galling. It maintains decent strength up to temperatures of 1800°F and has oxidation resistance similar to that of 309 stainless steel. The general corrosion resistance is between that of 304 and 316 stainless steel.
N60 Stainless
N60 Round Bar
UNS S21800, ASTM A276
| Ni | Cr | Mn | Si | C | N | S | P | Fe | |
|---|---|---|---|---|---|---|---|---|---|
| MIN | 8.0 | 16.0 | 7.0 | 3.5 | - | 0.08 | - | - | - |
| MAX | 9.0 | 18.0 | 9.0 | 4.5 | 0.10 | 0.18 | 0.03 | 0.06 | Balance |
Density: 0.275 lb/inch3
Electrical Resistivity: 589 ohm circ-mil/ft
| Temperature, °F | 70 | 200 | 400 | 600 | 800 | 1000 | 1200 | 1400 | 1600 | 1800 |
| Coefficient of Thermal Expansion, in/in°F x 10-6 | - | 8.8 | 9.2 | 9.6 | 9.8 | 10.0 | 10.3 | 10.5 | 10.7 | 11.0 |
| Modulus of Elasticity, psi X 106 STA |
- | 26.2 | - | - | - | - | - | - | - | - |
* 70°F to indicated temperature.
Minimum Specified Properties, ASTM A 276 Bar
| Ultimate Tensile Strength, ksi | 95 |
| 0.2% Yield Strength, ksi | 50 |
| Elongation, % | 35 |
| Reduction of Area, % | 55 |
| Hardness MAX, Brinell | 241 |
Typical Tensile Properties Annealed Bar ¾ - 1"
| Temperature, °F | 68 | 200 | 400 | 600 | 800 | 1000 | 1200 | 1400 | 1600 |
| Ultimate Tensile Strength, ksi | 106.5 | 98.2 | 84.4 | 80.5 | 78.3 | 75.4 | 66.6 | 49.8 | 30.2 |
| 0.2% Yield Strength, ksi | 56.5 | 44.4 | 32.8 | 29.7 | 29.0 | 28.0 | 28.1 | 25.3 | 16.4 |
| Elongation, 2% | 61.7 | 63.3 | 64.0 | 59.6 | 65.5 | 52.2 | 48.2 | 47.1 | 72.8 |