HydroFluoric acid

Hydrofluoric acid (HF) is very corrosive and can react with many metals, including cast iron, to generate hydrogen gas. Common stainless steel types, like 304 and 316, are not resistant to HF at any concentration or temperature. Higher grades of stainless steel may have some resistance, but they can still be attacked locally. 

Corrosion rates in Hydroflouric Acid (HF)

AlloyNotesConcentration, %TemperatureTimeCorrosion RateRef
  CFmm/yrmils/yr
316 — 3 21 70 — 1.25 49.1 1
316 — 5 21 70 — 2.33 91.8 1
316 — 5 40 104 — 7.8 306 1
316 — 1 50 122 — 1.82 71.8 1
316 — 2 50 122 — 5.3 209 1
316 — 5 50 122 — 15.9 626 1
904L — 3 21 70 — 0.125 4.9 1
904L — 5 21 70 — 0.18 7.2 1
904L — 5 40 104 — 0.73 28.8 1
904L — 1 50 122 — 0.23 9.2 1
904L — 2 50 122 — 0.71 28 1
904L — 3 50 122 — 0.85 33.5 1
904L — 4 50 122 — 1.36 53/5 1
904L — 5 50 122 — 1.82 71.6 1
904L — 1 70 158 — 0.99 39 1
904L — 2 70 158 — 2.0 80.2 1
904L — 3 70 158 — 3.31 130 1
AL-6XN — 3 21 70 — 0.08 3.2 1
AL-6XN — 5 21 70 — 0.20 8.0 1
AL-6XN — 5 40 104 — 0.82 32.4 1
AL-6XN — 1 50 122 — 0.10 4.1 1
AL-6XN — 2 50 122 — 0.43 16.9 1
AL-6XN — 3 50 122 — 0.98 38.4 1
AL-6XN — 4 50 122 — 1.42 55.9 1
AL-6XN — 5 50 122 — 2.0 78.7 1
AL-6XN — 1 70 158 — 0.54 21.1 1
AL-6XN — 2 70 158 — 1.98 78 1
AL-6XN — 3 70 158 — 3.05 120 1
C-276 — 2 70 158 — 0.23 9 7
C-276 — 5 70 158 — 0.25 10 7
C-22 — 2 70 158 — 0.23 9 7
C-22 — 5 70 158 — 0.36 14 7
625 — 2 70 158 — 0.51 20 7
625 — 5 70 158 — 0.41 16 7
400 saturated with air 25 30 86 24hr 1 37 17
400 saturated with air 25 80 176 24hr 0.28 11 17
400 saturated with air 50 30 86 24hr 0.2 8 17
400 saturated with air 50 80 175 24hr 1 39 17
400 purged with nitrogen 25 30 86 48hr 0.005 0.2 17
400 purged with nitrogen 25 80 176 48hr 0.061 2.4 17
400 purged with nitrogen 50 30 86 48hr <0.003 <0.1 17
400 purged with nitrogen 50 80 176 48hr 0.01 0.5 17