How to Weld Duplex Stainless Steel

basic rules and guidelines to help minimize issues

Rolled Alloys Metallurgical Services often receive questions about welding duplex stainless steel and general rules to follow to maintain corrosion resistance and properly preserve mechanical properties.

This article will discuss basic rules and guidelines to help minimize potential issues that may arise when welding duplex stainless steel. For in-depth details such as shielding gases, amperage, voltage, and other parameters, please consult the welding manuals for Zeronยฎ 100, 2205, and LDX 2101ยฎ.

Links for each grade's data sheet are found below:

Filler Metal

When welding, it is common practice to utilize a matching filler metal to that of the base material. Below is a table that shows the matching filler metal for various duplex grades.ย 

Base Material ย ย ย ย ย ย ย ย ย ย  Filler Metal

Zeronยฎ 100ย  ย  ย  ย  ย  ย  ย  Zeronยฎ 100X

2507 ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย  ER2594

2205 ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย ย  2209

LDX 2101ยฎย  ย  ย  ย  ย  ย  ย  ย  ย LDX 2101ยฎ

These filler metals are nearly identical in chemistry to their matching base metal, except for an additional 1.5 to 3% nickel, depending on the alloy. The higher nickel content aids in forming the 50/50 mix of austenite and ferrite phases. The benefit of these over-alloyed fillers is that there is no need for post-weld heat treatment. Additionally, it is common to see fabricators deviate from published matching filler metals due to either availability or additional corrosion resistance. For example, LDX 2101ยฎ is often welded with 2209 filler metal because it is more readily available. Also, higher nickel, chromium, and molybdenum filler metals increase corrosion resistance. To assist in weld wire selection for dissimilar metal welding,

Rolled Alloys provides a weld wire selector to assist with wires selection which can be accessed via the link below:

Weld Wire Selector

When dealing with specialty alloys, there can be unique welding combinations where guidance is not easily found. Let us help you take guesswork out of the equation.

Heat Input and Interpass Temperatures

By far, the most common error seen when welding duplex stainless steel is utilizing an improper heat input and interpass temperature. Duplex stainless steels require relatively high heat input and low interpass temperatures when welding to obtain the proper phase balance in the weld metal. ย Insufficient time at temperature can result in high ferrite and insufficient austenite. Conversely too much time at temperature can result in high austenite, an increased chance of forming nitrides and sigma phase in the base metal. These changes will decrease the corrosion resistance and toughness.

Quality Checks

It is essential to perform quality checks after welding to ensure proper phase balance. Therefore, when developing a welding procedure, it is critical to test corrosion resistance, impact toughness, and ferrite/austenite mix in the weld qualification to ensure that the final production weld yields good results and is fit for service. Often it is unfeasible to test a production weld thoroughly. As this is the case, it is common to utilize a ferritscope to test the ferrite content of a production weld to roughly determine any weld-related problems. Typically, incorrect ferrite levels will be the first indication of a problem. If a problem is found, further testing should be performed.ย  The ferritiscope is not a substitute for the more accurate microscopic methods.ย  Rather it is meant only as a QC check.ย  If there are inconsistencies, a destructive test and a microscopic investigation may be necessary.

Never Miss an Update - Subscribe Today!

Get application insights, material guides, and technical answers straight from the leaders in high-performance alloys.โ€‹

Share:

QUOTE, BUY, TRACK

We make it easy to get instant pricing and purchase your metal at the click of a button. Track your order progress, get notified when it ships, and follow your shipment online until it’s delivered. It’s that easy!

Latest Articles

5-Axis Waterjet Beveling

A 5-axis waterjet cutting machine is an advanced CNC cutting tool that uses a high-pressure stream of water mixed with abrasive (usually garnet) to cut through metals and other materials.

Read More ยป
Privacy Overview

This website uses cookies so that we can provide you with the best user experience possible. Cookie information is stored in your browser and performs functions such as recognising you when you return to our website and helping our team to understand which sections of the website you find most interesting and useful.