RA 253 MA® vs 309/310

RA 253 MA® Advantages Against 309/310: Overview

The main difference between RA 253 MA and both 309 and 310 stainless steel lies in alloy composition and resulting high‑temperature performance. RA 253 MA contains micro‑alloy additions of cerium, silicon, and nitrogen, which enhance oxidation resistance and creep strength at elevated temperatures. In addition, RA 253 MA has a lower overall nickel and chromium content, making it less susceptible to fluctuations in commodity pricing when compared to 309 and 310 stainless steels.

Key Differences and Comparisons

  • Alloying Elements and Cost Stability
    RA 253 MA includes additions of cerium, silicon, and nitrogen, while also having lower nickel and chromium content than 309 and 310 stainless steel. This lower alloy content makes RA 253 MA less vulnerable to fluctuating commodity prices.
  • Oxidation Resistance
    The micro‑alloy addition of cerium, along with silicon, provides RA 253 MA with good oxidation resistance up to 2000°F. This performance is comparable to 310 stainless steel and superior to 309 stainless steel.

  • Creep Strength at High Temperatures
    Due to the combined additions of carbon and nitrogen, the creep strength of RA 253 MA is more than twice that of both 309 and 310 stainless steel at temperatures above 1600°F.

  • ASME Pressure Vessel Approval
    RA 253 MA is approved under ASME Section VIII, Division 1 for pressure vessels up to 1650°F. In contrast, 309 and 310 stainless steels are only approved up to 1500°F.

  • ASME P-Group Classification
    RA 253 MA, 309, and 310 are all assigned to the same P‑Group in ASME Section IX: P‑Group 8, Group 2.

  • Welding Consumables for Matching Strength
    RA 253 MA is welded using RA 253 MA matching composition weld filler, available from Rolled Alloys in FCAW, GTAW, GMAW, and SMAW forms.

  • Dissimilar Metal Welding
    RA 253 MA can also be welded to other 300‑series stainless steels using RA 253 MA weld filler, or to higher‑nickel alloys using RA 333 weld filler, to maintain weld strength similar to the RA 253 MA base metal.

  • Product Availability
    Rolled Alloys stocks a complete range of RA 253 MA products, including plate, sheet, round bar, pipe, and welding consumables.

Chemical Composition %

 Cr Ni Si Mn N C Ce Fe
RA 253 MA® UNS S30815 21.0 11.0 1.7 0.6 0.2 0.08 0.04 balance
310 UNS S31008 25.0 20.0 0.5 1.6 -- 0.05 -- balance
309 UNS S30908 23.0 13.0 0.8 1.6 -- 0.05 -- balance

Creep-Rupture Properties

Minimum Creep Rate 0.0001% Per Hour

Stress to Rupture 10,000 Hours

Creep Test

Ring specimens subjected to a temperature of 1800°F under the stress of their own weight for a total of 32 hours.

See Figure to Left

Typical Tensile Properties, Plate

 Temperature 70°F 1200°F
RA 253 MA® Ultimate Tensile Strength, ksi 87 56.4
0.2% Offset Yield Strength ksi 45 23.0
310 Ultimate Tensile Strength, ksi 75 54.1
0.2% Offset Yield Strength ksi 30 20.7
309 Ultimate Tensile Strength, ksi 75 52.0
0.2% Offset Yield Strength ksi 30 22.0

ASME Section VIII Div. 1 Maximum Design Allowable Stresses

 Temperature °F 1100 1200 1350 1500 1650
RA 253 MA® ksi 9 5.2 2.4 1.3 0.71
310H ksi 7.6 4 1.7 0.75 --
309H ksi 7.6 4 1.4 0.75 --

309H and 310H are only approved to 1500°F. Values for 309H and 310H are used in this comparison as they have higher values than 309 and 310 straight grade. 

Maximum Suggested Temperature Limit in Air

2000°F Cyclic Oxidation Testing in Air

Contact Us!

Nick Hicks

Technical Marketing Manager

Garrett Gueldenzoph

Applications Engineer

Brennan Langdon

Applications Engineer

Never Miss an Update - Subscribe Today!

Get application insights, material guides, and technical answers straight from the leaders in high-performance alloys.​

Share:

QUOTE, BUY, TRACK

We make it easy to get instant pricing and purchase your metal at the click of a button. Track your order progress, get notified when it ships, and follow your shipment online until it’s delivered. It’s that easy!

Latest Articles